性能項目
|
試驗條件[狀態(tài)]
|
測試方法
|
測試數(shù)據(jù)
|
數(shù)據(jù)單位
|
吸水率
|
24小時浸漬(23℃)
|
ASTM D-570
|
DAM|50%RH,1.2|-
|
%
|
吸水率
|
飽和(23℃)
|
ASTM D-570
|
DAM|50%RH,8.5|-
|
%
|
比重
|
|
ASTM D-792
|
DAM|50%RH,1.14|1.14
|
泰伯磨耗量
|
cs-17 Wheel 1000g
|
|
DAM|50%RH,-|7
|
mg/1000 cycles
|
埃佐沖擊強度
|
23℃
|
ASTM D-256
|
DAM|50%RH,53|112
|
j/m
|
洛氏硬度M
|
|
ASTM D-785
|
DAM|50%RH,M79|M59
|
硬度計硬度
|
|
ASTM D-676
|
DAM|50%RH,89|82
|
洛氏硬度R
|
|
ASTM D-785
|
DAM|50%RH,R121|R108
|
屈服強度
|
23℃
|
|
DAM|50%RH,82.7|58.6
|
MPa
|
拉伸強度
|
23℃
|
ASTM D-638
|
DAM|50%RH,82.7|77.2
|
MPa
|
揉曲模量
|
23℃
|
ASTM D-790
|
DAM|50%RH,2827|1207
|
MPa
|
拉伸沖擊強度
|
短試樣23℃
|
ASTM D-1822
|
DAM|50%RH,157|231
|
KJ/m2
|
1%形變時的壓應(yīng)力
|
|
ASTM D-695
|
DAM|50%RH,33.8|-
|
MPa
|
剪切強度
|
23℃
|
ASTM D-732
|
DAM|50%RH,66.2|-
|
MPa
|
斷裂伸長率
|
23℃
|
ASTM D-638
|
DAM|50%RH,60|≥300
|
%
|
屈服伸長率
|
|
ASTM D-638
|
DAM|50%RH,5|25
|
%
|
拉伸沖擊強度
|
長試樣23℃
|
ASTM D-1822
|
DAM|50%RH,504|1470
|
KJ/m2
|
介電常數(shù)
|
106Hz(cps)
|
ASTM D-150
|
DAM|50%RH,3.6|4.6
|
耗散因數(shù)
|
100Hz(cps)
|
ASTM D-150
|
DAM|50%RH,0.01|0.2
|
介電常數(shù)
|
103Hz(cps)
|
ASTM D-150
|
DAM|50%RH,3.9|7.0
|
耗散因數(shù)
|
106Hz(cps)
|
ASTM D-150
|
DAM|50%RH,0.02|0.1
|
耗散因數(shù)
|
103Hz(cps)
|
ASTM D-150
|
DAM|50%RH,0.02|0.2
|
體積電阻率
|
|
ASTM D-257
|
DAM|50%RH,10,15,|10,13
|
Ω.cm
|
介電常數(shù)
|
100Hz(cps)
|
ASTM D-150
|
DAM|50%RH,4.0|8.0
|
荷重形變
|
13.8MPa,50℃
|
ASTM D-621
|
DAM|50%RH,1.4|-
|
%
|
熱畸變溫度
|
18×106Pa
|
ASTM D-648
|
DAM|50%RH,90|-
|
℃
|
熔點結(jié)晶
|
|
ASTM D-2177
|
DAM|50%RH,270|-
|
℃
|
UL可燃性導(dǎo)級
|
|
UL 94
|
DAM|50%RH,94|V-2
|
脆化溫度
|
|
ASTM D-746
|
DAM|50%RH,-80|-65
|
℃
|
熱畸變溫度
|
(0.5)×106Pa
|
ASTM D-648
|
DAM|50%RH,235|-
|
℃
|
導(dǎo)熱系數(shù)
|
|
|
DAM|50%RH,0.25|-
|
w/mk
|
線性熱膨脹系數(shù)
|
|
ASTM D-696
|
DAM|50%RH,7×10,-5,|-
|
m/m/℃
|
熔點
|
Fisher Johns法
|
ASTM D-789
|
DAM|50%RH,255|255
|
℃
|
需氧指數(shù)
|
|
ASTM D-2863
|
DAM|50%RH,28|31
|
%
|
|